Wire electrode for
Welding Unalloyed and Low-alloy Steels |
|
|
|
|
Standards: |
EN 440 |
G 46 4 M G4
Si 1 |
|
DIN 8559
|
SG 3 CY 46
43 |
|
AWS/ASME SFA
5.18 |
ER 70 S - 6
|
|
TS 5618
|
SG 3 CY 46
43 |
|
M.No.
|
1.5130
| |
|
Application and Properties: |
Unalloyed welding
electrode for GMA (MAG) welding of general structural
steels and pipe steels using CO2 or mixed shielding gas.
Preheating is required, depending on the plate thickness
and carbon equivalent of the base metal. A thin and
homogeneous copper coating increases electrical
conductivity and protects the wires from
rusting. |
|
Materials:
|
S185 |
St 33 |
S235 - S355 |
St 37.0 - St 52.0
|
S235 - S355 |
St 37-2 - St 52-3
|
P235 - P355 |
St 37.4 - St 52.4
|
P235 |
St 35.8 |
P265 |
St 45.8 |
P235GH , P265GH
|
HI, HII |
P295GH , P355GH
|
17 Mn 4, 19 Mn 5
|
E295, E335 |
St 50, St 60*
|
L210 - L360 |
StE210.7(TM) -
StE360.7(TM) |
- |
GS-38, GS-52
|
GP240R |
GS-45 |
- |
A, B, D, E |
- |
StE 285 - StE 460
|
|
*Preheat to 150-300˚C,
depending on the plate thickness. |
|
Qualification
Tests |
: TSE
| |
|
All-Weld
Metal Analysis (typical values in %) : |
0.08 |
0.90 |
1.70 |
<0.025 |
<0.025 |
|
|
Mechanical
Properties of All-Weld Metal (single values are typical
values): |
|
AW : As welded |
|
Chemical
compositions and mechanical properties apply to
the use of shielding gas |
|
: EN
439 - C1 (100% CO2) | |
|
Shielding gas
as to EN 439 |
: C1 (100% CO2),
M21, M22, M23, M24 | |
|
Shielding gas
consumption |
: 12 l/min for Ø
0.8 mm, 15 l/min for Ø 1.2 mm
| |
|
Packing
& Order Information : |
2013001 |
0.80 |
15 |
2013003 |
1.00 |
15 |
2013005 |
1.20 |
15 |
2013007 |
1.40 |
15 |
2013008 |
1.60 |
15 |
2013010 |
2.40 |
15 |
|
|
Type of
Current/Polarity/Welding Positions : |
You can click on